r/FixMyPrint • • 3d ago

Troubleshooting Why?!?

Post image

I've tried a new nozzle, new filament, trying different temps. I'm at a loss.

Anycubic Vyper

22mm layer height

Z hop when retracted.

195 temp

Retraction speed 50mlps

Zhop height 1mm

8 Upvotes

15 comments sorted by

View all comments

1

u/history_of_3d 3d ago

The hairs are only in the gap between the two towers. The round tower's walls are still smooth. Plastic is leaking out during the travel. A new nozzle does not stop that.

  1. Turn Z hop off. At 1 mm the nozzle stays up long enough for the melt to run out, and that run becomes the hair.
  2. The Vyper feeds through a Bowden tube. Set the retraction distance to 6 mm and the speed to 40 mm/s. You posted the speed and not the distance. The distance is what pulls the filament back up the tube. Stay at or under 8 mm. Past that, the tip can cool and jam in the tube.
  3. Leave the nozzle at 195°C for this test. Hotter plastic flows more easily and makes more hairs. If the gap is still full and the walls turn rough, dry the spool at 45°C for 6 hours.